結構膠混合不均勻,局部會出現白色條紋。在光線比較亮的情況下,更加容易觀察。混合不均勻和混合均勻的情況,結構膠固化后的強度下降,固化交聯不完全、嚴重時候會發粘,無法固化等。那么雙組份打膠機出現結構膠混合不均的情況是什么原因造成的呢?我們又該如何避免呢?
Structural adhesives are unevenly mixed and white stripes appear locally. It is easier to observe when the light is brighter. When the mixing is not uniform and the mixing is uniform, the strength of the structural adhesive decreases after curing, the curing cross-linking is incomplete, and when the curing is serious, it will stick and can not be cured. So what is the reason for the uneven mixing of structural glue in the two-component glue beater? How can we avoid it?
混合不均勻的結構膠有以下四種情況及原因如下:
There are four kinds of uneven mixing structural adhesives and the reasons are as follows:
①連續花膠:一般是混合器堵塞、混合器裝配錯誤或者使用的混合單元不夠多;
(1) Continuous gum: generally, the mixer is blocked, the mixer assembly is wrong or the mixing unit is not enough;
②斷續有規律花膠:與系統性故障有關,如配比泵密封泄漏或者比例架磨損;
(2) Intermittent regular pattern gum: related to systemic faults, such as leakage of seal of proportioning pump or wear of proportioning frame;
③斷續無規律花膠:與故障有關,如過濾器堵塞/針閥堵塞/壓盤故障/配比泵入口堵塞或者密封失效/閥及高壓球閥失效等;
(3) Discontinuous irregular pattern gum: related to faults, such as filter blockage/needle valve blockage/platen failure/ratio pump entrance blockage or seal failure/safety valve and high pressure ball valve failure;
 
雙組份打膠機
④短暫停槍后又開槍時,開頭出現一段花膠:主要是膠粘度匹配不理想,需要調整系統管道或降低工作壓力。
(4) When the gun stops for a short time and fires again, a section of gum appears at the beginning: the main reason is that the gum viscosity matching is not ideal, and the system pipeline needs to be adjusted or the working pressure should be reduced.
要避免這種情況的出現,我們要對打膠機要定期進行保養,確保打膠機可以正常工作。每次開機前必須做蝴蝶試驗,確保結構膠混合均勻。蝴蝶試驗的方法如下:將打膠機打出的混合好的膠擠到紙中間5-10克,折合紙將膠壓平。打開紙檢查膠樣,混合均勻的膠應無異色條紋,如果膠出現異色條紋,則表明混膠不均勻,應查找原因,問題解決后才能使用。
To avoid this situation, we need regular maintenance of the glue machine to ensure that the glue machine can work properly. Butterfly test must be done before starting each machine to ensure that the structural glue mixes evenly. The butterfly test method is as follows: the mixed glue produced by the gluer is squeezed into the middle of the paper for 5-10 grams, and the folding paper is pressed flat. Open the paper and check the rubber sample. The glue with uniform mixing should have no heterochromatic stripes. If there are heterochromatic stripes in the glue, it shows that the mixing is not uniform. The reason should be found out and the problem can be solved before using it.
以上就是由雙組份打膠機的小編給大家整理提供的精彩內容了,想要了解更多詳情,歡迎大家收藏我們官網:http://m.vrqf.com.cn
The above is the wonderful content provided to you by the small edition of the two-component glue machine. For more details, you are welcome to collect our official website: http://m.vrqf.com.cn

上一篇:雙組份打膠機知液灌膠機的清洗辦法
下一篇:中空玻璃設備生產線使用注意事項

  • 微信
主站蜘蛛池模板: 国产视频你懂的 | 国产成人自啪精品视频 | 欧美影片一区二区三区 | 黄色激情视频在线观看 | 国产亚洲欧美久久久久 | 日本欧美一区二区三区视频 | 中文精品久久久久国产网站 | 日韩欧美一区二区三区在线视频 | 国产不卡精品一区二区三区 | 国产在线观看网址在线视频 | 亚洲国产成人最新精品资源 | 天堂视频在线免费观看 | jk制服啪啪网站 | 香港午夜伦理 | 中文字幕亚洲精品资源网 | 成年黄网站在线观看免费 | 欧美性受一区二区三区 | 免费观看91视频 | 一本视频在线 | 国产精品98视频全部国产 | 最近日本中文字幕免费完整 | 欧美成a人片免费看久久 | 99精品国产成人一区二区 | 国产亚洲欧美日韩综合综合二区 | 亚洲日本va中文字幕久久 | 欧美特黄a级高清免费看片 欧美特黄a级高清免费大片 | 国精产品一区一区三区 | 日本中文字幕视频 | 欧美国产激情二区三区 | 欧美精品一线二线大片 | 国产一区二| 亚洲无线码一区二区三区在线观看 | 久久精品免费观看 | 国产精品一区二区在线观看 | 在线成人影视 | 在线观看你懂的网站 | 暴力调教抖s浪荡总裁受文 白洁性荡生活l六 | 久久夜夜肉肉热热日日 | 五月天亭亭| 北条麻妃初尝试黑人在线观看 | 天天做天天添天天谢 |